Skip to main navigation Skip to search Skip to main content

Investigation into the effect of varying aluminium surface pre-treatments on the mechanical properties of hybrid aluminium-carbon fibre reinforced plastics joints

  • Raja Muhamad Hafiz Raja Adzhar

    Abstract

    In high-performance sectors such as aerospace, automotive, and structural engineering, joining dissimilar materials like aluminium and carbon fibre reinforced plastic (CFRP) is essential for achieving lightweight structures with high strength and controlled deformation. This research investigates the design, manufacture, and testing of Al–CFRP hybrid joints with various aluminium surface pre-treatments: untreated, micro blasted, etched, crystallised, and machined pins.
    Mechanical characterisation was conducted using Mode I (double cantilever beam) and Mode II (lap shear) tests to assess fracture toughness and shear strength, respectively. The study identifies two primary mechanisms influencing joint performance: chemical bonding and mechanical interlocking, with their effectiveness dependent on the loading mode.
    In Mode I, chemical bonding plays a dominant role. Etching enhances adhesion by introducing hydroxyl (-OH) groups, while crystallisation forms nano-needle boehmite structures that increase surface energy and nanoscale interlocking. These treatments significantly improved fracture toughness (Gic), with the micro blasted and crystallised pin (PMBC) design achieving the highest performance of >4 N/mm, representing an improvement of approximately 1,900% over the untreated sample.
    In Mode II, mechanical interlocking is the main contributor to the joint strength. Micro blasting increases surface roughness and frictional resistance, resulting in the micro blasted pin (PMB) sample achieving the highest shear strength of >16 MPa, approximately 300% higher than the untreated sample. Although chemical treatments alone had limited impact under shear loading, combining them with mechanical roughening and through-thickness reinforcement (TTR) provided collaborative effects. The PMBC joint showed the highest strain capacity (18.30%) while maintaining strong shear performance (13.57 MPa), indicating enhanced loadbearing capacity and failure resistance.
    This research concludes that optimising the balance between chemical and mechanical bonding mechanisms is critical for improving Al–CFRP joint performance. The PMBC configuration emerges as the most effective hybrid design, offering enhanced toughness, strength, and durability, and shows strong potential for future lightweight structural joining applications.
    Date of Award24 Jul 2025
    Original languageEnglish
    Awarding Institution
    • Northumbria University
    SupervisorMartin Birkett (Supervisor) & Matthew Blacklock (Supervisor)

    Keywords

    • Crystallisation
    • Double cantilever beam test (Mode I)
    • Lap shear test (Mode II)
    • Fracture toughness and strength of dissimilar materials joint
    • Mechanical and chemical interactions of dissimilar materials joint

    Cite this

    '